A model for predicting surface topography following nanosecond pulsed laser texturing of metals is applied to calculating the areal surface roughness, Sa, average ablation depth, Da, and Wenzel roughness factor or adhesion area ratio,r, for a range of representative cases relating to adhesion and wettability. Optimisation of the laser scanning strategy, number of laser passes and focused spot size is performed by considering the ratio of increases in Sa and rwith respect to the average ablation depth: Sa/Daand Δr/Da, where Δr = r - 1. Highest values of Sa Da/ and Δr/Da are achieved where the pulse separation distance is equal to the focused spot size in both the scanning and lateral directions. Increases in Sa,r and Δr/Da can be achieved by performing multiple laser passes, while r and Δr/Da can be increased independently of Sa and Sa/Da by reducing the focused laser spot size. These results suggest thatr and Sa can be optimised effectively and independently in line with a given application. Finally, laser texturing experiments are performed on AA 6082 aluminium alloy and 316L austenitic stainless steel specimens with the aim of confirming model outcomes, after which tensile tests are performed on adhesive-bonded joints prepared with the same laser treatments. Further to demonstrating the benefits of laser texturing, it is shown that optimum results are not necessarily associated with a single value of Sa orr, but are instead a compromise between maximising these parameters and limiting the ablated volume.
Surface topography following pulsed laser texturing: Implications for adhesion and wettability / Lutey, A. H. A.; Romoli, L.. - In: SURFACE TOPOGRAPHY. - ISSN 2051-672X. - 7:4(2019), p. 045023. [10.1088/2051-672X/ab5c82]
Surface topography following pulsed laser texturing: Implications for adhesion and wettability
Lutey A. H. A.
;Romoli L.
2019-01-01
Abstract
A model for predicting surface topography following nanosecond pulsed laser texturing of metals is applied to calculating the areal surface roughness, Sa, average ablation depth, Da, and Wenzel roughness factor or adhesion area ratio,r, for a range of representative cases relating to adhesion and wettability. Optimisation of the laser scanning strategy, number of laser passes and focused spot size is performed by considering the ratio of increases in Sa and rwith respect to the average ablation depth: Sa/Daand Δr/Da, where Δr = r - 1. Highest values of Sa Da/ and Δr/Da are achieved where the pulse separation distance is equal to the focused spot size in both the scanning and lateral directions. Increases in Sa,r and Δr/Da can be achieved by performing multiple laser passes, while r and Δr/Da can be increased independently of Sa and Sa/Da by reducing the focused laser spot size. These results suggest thatr and Sa can be optimised effectively and independently in line with a given application. Finally, laser texturing experiments are performed on AA 6082 aluminium alloy and 316L austenitic stainless steel specimens with the aim of confirming model outcomes, after which tensile tests are performed on adhesive-bonded joints prepared with the same laser treatments. Further to demonstrating the benefits of laser texturing, it is shown that optimum results are not necessarily associated with a single value of Sa orr, but are instead a compromise between maximising these parameters and limiting the ablated volume.I documenti in IRIS sono protetti da copyright e tutti i diritti sono riservati, salvo diversa indicazione.